hardrockminer wrote:

katit wrote: Got my kit! Realized I need a heater. Read some people use aquarium tank heaters. Can anyone point to heater they use and how does it work?


I use an aquarium heater but can't recall the brand. I also use a thermometer.


I am trying to find appropriate aquarium heater but so far only one comes close (size-wize) because of bucket size. Those sticks pretty tall when powerful.
Do you know how many watts your heater is? And how long does it take to bring solution up to temp? Or do you use something else to heat it and then use aquairum heater to maintain only?


78 KZ650B2A - resto in progress
www.kzrider.com/forum/11-projects/615161...s-1978-kz650-project
Other bikes: 1978 BMW R100/7, 1978 Moto Guzzi T3, 2016 DRZ400s

Please Log in or Create an account to join the conversation.

More
25 Jan 2021 12:51 #842386 by Nessism
Replied by Nessism on topic Plating at home
I need a new heater but can't seem to find a decent one. Beware ordering a heater on Amazon because many of them are huge (I had to send two different ones back.)

Something in the 300W range is good, with a temp range of about 100F. Most aquarium heaters are lower temp than that. And many aquarium heaters are glass which is ripe for breakage.

Please Log in or Create an account to join the conversation.

More
25 Jan 2021 12:58 #842387 by katit
Replied by katit on topic Plating at home
No eBay APP ID and/or Cert ID defined in Kunena configuration

Nessism wrote: I need a new heater but can't seem to find a decent one. Beware ordering a heater on Amazon because many of them are huge (I had to send two different ones back.)

Something in the 300W range is good, with a temp range of about 100F. Most aquarium heaters are lower temp than that. And many aquarium heaters are glass which is ripe for breakage.


Yes, I am still reading on it.. Many people use aquarium heaters but they go to 95F and solution need to be 110F I think.
I am thinking Sous Vide heater. Just not sure if they will survive in plating bath? It's all in one. Heater, circulator and precise temp control all in one.
Used to be expensive, now getting cheaper. I've see used ones locally for like $25. Use one for cooking - it does exactly what we need..


78 KZ650B2A - resto in progress
www.kzrider.com/forum/11-projects/615161...s-1978-kz650-project
Other bikes: 1978 BMW R100/7, 1978 Moto Guzzi T3, 2016 DRZ400s

Please Log in or Create an account to join the conversation.

More
26 Jan 2021 07:18 #842428 by katit
Replied by katit on topic Plating at home
No eBay APP ID and/or Cert ID defined in Kunena configurationNo eBay APP ID and/or Cert ID defined in Kunena configurationThis is my solution for heating. Should work but don't know how "precise" it will be. With heater like this I expect inertia swings.
Digital relay switch 15A (there is cheaper ones, but I figured I might use it later for other things)


And plain water heater:

78 KZ650B2A - resto in progress
www.kzrider.com/forum/11-projects/615161...s-1978-kz650-project
Other bikes: 1978 BMW R100/7, 1978 Moto Guzzi T3, 2016 DRZ400s

Please Log in or Create an account to join the conversation.

More
26 Jan 2021 16:43 #842472 by Nessism
Replied by Nessism on topic Plating at home
1000W heater is hot. That thing is 12" long too which will stick out above the fluid. Please provide a review of how it works out.

Back a few years ago Caswell's kits came with a thermostat unit and separate heaters. The heaters burned out but the thermostat still works. I bought a cheap 300W tea pot heater which is similar to yours only a good deal smaller. It worked okay, a bit slow to heat the bucket, but then it failed. I'm on the fence about what to buy next.
The following user(s) said Thank You: katit

Please Log in or Create an account to join the conversation.

More
04 May 2021 07:48 #847982 by katit
Replied by katit on topic Plating at home
Been about 3 month - finally got to use my kit.
First of all - controller/heater combo works great. Heats up in about 15 minutes (to 120F) and then keeps in within 2 degrees. Long heater does not hurt plastic, I guess where it touches on top there is not much heat. I touched with fingers. Hot, but not melting. I used simple metal rod thingy to hold it against the wall.

My prep was degrease, than bead blast in cabinet.

Then - per caswell manual. Degrease, acid dip, plate, chromate dip.

My observations/notes.

1. Degreasing bath. I don't have second heater. So, what I did - I used my heater to get it up to about 180 and than put all pre-wired pieces in and closed lid loosely (used  caswell provider bucket). I don't think it hurts to keep parts in there for 2hr (vs 5 min)

2. Per Nessism info - I dip in acid (mixed muriatic acid from HD 50/50 with distilled water) until bubbling stops. Probably 10-15 seconds, maybe more for some certain bolts.

3. Plating. I didn't calculate surface/amps. I went by looks. Circulator pump off. Increase amperage until I see slight bubbling from parts. Most batches were done between 1-2 amps according to my power supply. 17 minutes or so. 

4. Chromate. About 5 seconds in it. I mixed about 2qt of it total, plenty for all the bolts/nuts.

2 things I might want to improve but not sure..
A. Brightness/polish. I guess with wire wheel prep it will be brighter. But it will be too much work. Currently pieces semi-bright. From that regard they look perfect to me.
B. Color. Color is nice, but not for KZ. Original screws I purchased were more green/blue vs yellow. This is real dilemma now as I don't want to wait for postage from caswell with different chromate. I might just dip for 2 seconds and get very slight yellow in next batches.

Overall - easy. I just set timer and go to garage every 17 minutes for minute or two. If you do all the prep then there is not much else to do.

 

78 KZ650B2A - resto in progress
www.kzrider.com/forum/11-projects/615161...s-1978-kz650-project
Other bikes: 1978 BMW R100/7, 1978 Moto Guzzi T3, 2016 DRZ400s

Please Log in or Create an account to join the conversation.

More
04 May 2021 16:01 #848007 by Nessism
Replied by Nessism on topic Plating at home
Dip less time or dilute the yellow chromate more.  I'd do the later if your container allows it.  Also be sure to rinse off the chromate after dipping.
The following user(s) said Thank You: katit

Please Log in or Create an account to join the conversation.

More
04 May 2021 18:03 #848010 by 73z1
Replied by 73z1 on topic Plating at home
The gold parts are zinc dichromate.
Post photo of clear zinc if you plated.
I tried Caswell, your parts look nice.
 
The following user(s) said Thank You: katit

Please Log in or Create an account to join the conversation.

More
05 May 2021 07:45 - 05 May 2021 07:47 #848027 by katit
Replied by katit on topic Plating at home
Some more plating. Diluted chromate and started to rinse after chromate (didn't do it first time). But yesterday's batch started dull. Not sure why, but after adding half cap brightener and raising amps I started to get better results. On picture - before chromate - this is best I had yesterday. All shiny straight of plating bath.
Slow process, but it works. For some reason my "guess" on surface area were far from what I found in Caswell XLS table. I needed about 2.5A for those shiny bolts to plate. My guess was 1A but wrong.

You can see different shades of bling on those head nuts while I was adjusting with amps, etc. 

Questions:
1. I don't do acid dip (short) before chromate. Do you guys do it and is there difference? (manual says to do it)
2. How often do you add brightener? 
3. Amps. How do you manage those? By looking at parts bubbling? Or calculate with formula(pain)?
4. Chromate. I noticed if it's dry but not for long, it comes off with my fingers from shiny parts. Does it have to dry for long? Or it's issue with process?

 

78 KZ650B2A - resto in progress
www.kzrider.com/forum/11-projects/615161...s-1978-kz650-project
Other bikes: 1978 BMW R100/7, 1978 Moto Guzzi T3, 2016 DRZ400s
Last edit: 05 May 2021 07:47 by katit.

Please Log in or Create an account to join the conversation.

More
05 May 2021 08:32 #848033 by Nessism
Replied by Nessism on topic Plating at home
Acid dip before chromate is good but short time.  Get a medium fizz going then stop and rinse.  Acid solution should be pretty weak.

Add brightener when parts are dull.  Too much brighter will give the parts a slight brown cast.

I add current based on fizz..

Chromate is fragile but that improves when dry.

Please Log in or Create an account to join the conversation.

More
05 May 2021 08:56 #848036 by katit
Replied by katit on topic Plating at home

Add brightener when parts are dull.  Too much brighter will give the parts a slight brown cast.

 
How fast do you go through brightener? Just wanted to make sure I don't run out before finish, takes couple weeks to get stuff from Caswell. Will included bottle last through bike worth of parts?

78 KZ650B2A - resto in progress
www.kzrider.com/forum/11-projects/615161...s-1978-kz650-project
Other bikes: 1978 BMW R100/7, 1978 Moto Guzzi T3, 2016 DRZ400s

Please Log in or Create an account to join the conversation.

More
05 May 2021 20:20 - 06 May 2021 05:02 #848066 by Nessism
Replied by Nessism on topic Plating at home
To be honest, I struggle with the brightness of my plated parts at times.  When the electrolyte is new the parts come out much brighter, and when adding brightener I use maybe 1 oz. at a time.  I'm not sure why the dullness sets in but if the parts are particularly dull I use a dremel with a stainless wire wheel of some time and give the parts a little buff job.  That brings up the shine to an acceptable level.
Last edit: 06 May 2021 05:02 by Nessism.